Presintered Ferrite powder YXC Specification of YXC Dry Pressing Strontium Ferrite Magnetic Materials
YXC series Strontium Dry Pressing Ferrite Magnetic Powders are suitable for producing magnets by dry pressing. According to the requirement , such products can be classified as isotropic powder and anisotropic powder , anisotropic powder has better orientability. The strict quality control system ensures that the quality is stable and reliable.
1. YXC series Dry Pressing Strontium Ferrite Material Properties
Type
|
Br
|
Hcb
|
Hcj
|
(BH)max
|
Sintered density
|
Grade
|
mT
|
Gs
|
KA/m
|
Oe
|
KA/m
|
Oe
|
KJ/m3
|
MGOe
|
P(g/cm3)
|
YXC-C1T
|
230
|
2300
|
150
|
1880
|
240
|
3010
|
9.50
|
1.19
|
4.6+/-0.2
|
YXC-C2T
|
230
|
2300
|
155
|
1950
|
278
|
3500
|
9.60
|
1.20
|
4.6+/-0.2
|
YXC-C3T
|
210
|
2100
|
150
|
1880
|
350
|
4400
|
9.00
|
1.13
|
4.6+/-0.2
|
YXC-C1
|
370
|
3700
|
215
|
2700
|
231
|
2900
|
24.6
|
3.08
|
4.6+/-0.2
|
YXC-C2
|
385
|
3850
|
219
|
2750
|
231
|
2900
|
26.0
|
3.27
|
4.6+/-0.2
|
YXC-C3
|
395
|
3950
|
231
|
2900
|
235
|
2950
|
28.8
|
3.60
|
4.6+/-0.2
|
2. YXS series Dry Pressing Barium Ferrite Material Properties.
Trade Mark
|
Material
|
Characteristics of products
|
Granularity
|
Forming methods
|
Br(mT)
|
bHc(kA/m)
|
ihc(kA/m)
|
(BH)max(kJ/m3)
|
SHR%
|
Pellets
(mm)
|
Coarse
Powder
(¦Ìm)
|
Fine powder
|
Typical
|
Min
|
Typical
|
Min
|
Typical
|
Min
|
Typical
|
Min
|
YXS-1
|
BaFe12O19
|
225
|
220
|
143
|
139
|
215
|
199
|
7.96
|
7.56
|
15¡À1
|
6-12
|
3-6
|
0.80-0.90
|
Isotropic dry press
|
195
|
190
|
123
|
119
|
215
|
199
|
5.57
|
5.17
|
15¡À1
|
YXS-1R
|
BaFe12O19
|
230
|
225
|
143
|
139
|
255
|
239
|
8.36
|
7.96
|
15¡À1
|
6-12
|
3-6
|
0.80-0.90
|
215
|
210
|
135
|
131
|
255
|
239
|
7.56
|
7.16
|
15¡À1
|
YXS-1A
|
BaFe12O19
|
235
|
230
|
147
|
143
|
239
|
223
|
8.75
|
8.36
|
15¡À1
|
6-12
|
3-6
|
0.80-0.90
|
200
|
195
|
127
|
123
|
239
|
223
|
5.97
|
5.57
|
15¡À1
|
3.Procedure Summaries
There are 6 types of dry pressing ferrite powder for customers:YXC-C1,YXC-C2T,YXC-C3T,YXC-C1,YXC-C2.The procedure summaries for making magnet are as follows:
a. The necessary secondary additives have been added into the powder during the grinding process.Customers shall only add proper quantity of binders and lubricants.The powder must pass through 120 mesh sieve before pressing,so as binders to be uniformly distributed for better orientaton.
b.Please take care of the cleaning of the equipments.Any other materials and impurity should mot be mixed into the powder.
c.During pressing,the pressure required is >=5000N/cm2,and the magnetic field density is >7000 Oe(560KA/m).
d.The sintering temperature for reference is 1220OC to 1270 OC.Please note that the proper sintering temperature should be defined in accordance with the status of the sintered sample pill. |
Specifications of YXC Wet pressing Strontium Ferrite Magnetic Materials
YXC series strontium Ferrite Magnetic powders have been designed to produce all grades of hard ferrites.The users will make high quality magnets by adding the provided additives into the powders.Our highly automatic instruments and strict quality control system ensure that the quality is stable and reliable.
a. Material Properties
Trade Mark
|
Material
|
Characteristics of products
|
Granularity
|
Forming methods
|
Br(mT)
|
bHc(kA/m)
|
ihc(kA/m)
|
(BH)max(kJ/m3)
|
SHR %
|
Pellets(mm)
|
Coarse Powder (¦Ìm)
|
Fine powder
|
Min
|
Typical
|
Min
|
Typical
|
Min
|
Typical
|
Min
|
Typical
|
YXS-2.4B
|
SrFe12O19
|
380
|
370
|
183
|
167
|
199
|
183
|
27.1
|
25.5
|
15.5¡À1
|
¡¡
|
|
0.80-0.90
|
Anisotropic dry press
|
YXS-2.4
|
SrFe12O19
|
360
|
350
|
223
|
207
|
239
|
223
|
23.9
|
22.3
|
15.5¡À1
|
6-12
|
3-6
|
0.80-0.90
|
YXS2.4H
|
SrFe12O19
|
340
|
330
|
255
|
239
|
279
|
255
|
21.5
|
19.9
|
15¡À1
|
¡¡
|
|
0.80-0.90
|
YXS-2.4E
|
SrFe12O19
|
320
|
310
|
239
|
223
|
318
|
294
|
19.1
|
17.5
|
15¡À1
|
¡¡
|
|
0.80-0.90
|
YXS-2.5B
|
SrFe12O19
|
400
|
390
|
191
|
175
|
199
|
183
|
30.2
|
28.7
|
15.5¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-2.5
|
SrFe12O19
|
380
|
370
|
233
|
207
|
239
|
223
|
27.1
|
25.5
|
15.5¡À1
|
¡¡
|
|
0.80-0.90
|
YXS-2.5H
|
SrFe12O19
|
360
|
350
|
263
|
247
|
302
|
279
|
23.9
|
22.3
|
15¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-2.5E
|
SrFe12O19
|
340
|
330
|
255
|
239
|
342
|
318
|
21.5
|
19.9
|
15¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-2.5U
|
SrFe12O19
|
320
|
310
|
239
|
223
|
398
|
374
|
19.1
|
17.5
|
15¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-3
|
BaFe12O19
|
390
|
380
|
159
|
151
|
163
|
155
|
28.7
|
27.1
|
12¡À1
|
¡¡
|
¡¡
|
0.90-1.00
|
Anisotropic wet press
|
YXS-4B
|
SrFe12O19
|
410
|
400
|
191
|
175
|
199
|
183
|
31.8
|
30.2
|
13¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-4
|
SrFe12O19
|
390
|
380
|
231
|
215
|
239
|
223
|
28.7
|
27.1
|
13¡À1
|
6-12
|
3-6
|
0.80-0.90
|
YXS-4H
|
SrFe12O19
|
370
|
360
|
259
|
243
|
279
|
263
|
25.5
|
23.9
|
13¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-4E
|
SrFe12O19
|
350
|
340
|
259
|
243
|
318
|
294
|
23.1
|
21.5
|
12.5¡À1
|
¡¡
|
¡¡
|
0.80-0.90
|
YXS-5B
|
SrFe12O19
|
430
|
420
|
191
|
175
|
199
|
183
|
35.0
|
33.4
|
13¡À1
|
¡¡
|
¡¡
|
0.75-0.85
|
YXS-5
|
SrFe12O19
|
410
|
400
|
231
|
223
|
239
|
231
|
31.8
|
30.2
|
13¡À1
|
6-12
|
3-6
|
0.75-0.85
|
YXS-5H
|
SrFe12O19
|
390
|
380
|
283
|
267
|
302
|
279
|
28.7
|
27.1
|
13¡À1
|
6-12
|
3-6
|
0.75-0.85
|
YXS-5E
|
SrFe12O19
|
370
|
360
|
279
|
263
|
342
|
318
|
25.5
|
23.9
|
12.5¡À1
|
¡¡
|
¡¡
|
0.75-0.85
|
YXS-5U
|
SrFe12O19
|
350
|
340
|
263
|
247
|
398
|
374
|
23.1
|
21.5
|
12.5¡À1
|
¡¡
|
¡¡
|
0.75-0.85
|
YXS-6
|
SrFe12O19
|
410
|
400
|
271
|
255
|
279
|
263
|
31.8
|
30.2
|
12.5¡À1
|
¡¡
|
¡¡
|
0.70-0.80
|
YXS-6H
|
SrFe12O19
|
400
|
390
|
294
|
279
|
318
|
294
|
30.2
|
28.7
|
13¡À1
|
¡¡
|
¡¡
|
0.70-0.80
|
*The shrinkage rate on vertical direction is about 13¡À0.5%
2.In case that the granular material is pruchased from our company,the particle should be dry ground to 3-5¦Ìm at first,and then be wet ground in a sand grinding mill or ball mill to less than 1 ¦Ìm ,and then be wet pressed.If the coarse ground powder is bought,it can be wet ground directly.
1).Before grinding,the grinding mill should be cleaned thoroughly.And any materials from other factories or Impurity should not be mixed into our material.
2).Aloong with the powder (granular powder,and coarse ground powder),we provide the secondary additives in separated bags,users should only add it into powder during grinding according to the requirement.
3.All the necessary secondary additives have been added into the fine powders(<1¦Ìm).So there is no need to add any other material,But two to three hours'wet grinding is necessary for better distribution of particles.
4.During pressing,the moisture of slurry should be controlled between 32% to 37%,the pressure required is >4000N/cm2,and the magnetic field density is >560kA/m.
5.Due to the actual sintering temperature measured by various suppliers' instruments are not the same,we can only provide sintering temperature of 1220OC-1270OC for reference.Please note that the proper sintering temperature should be defined in accordance with the status of the sintered sample pill.
|